Production Process of GB 50 kg Heavy Rail

Apr 27, 2025 Leave a message

Steelmaking and Billet Preparation

The 50 kg/m heavy rail section is rolled from continuously cast blooms of high carbon steel in grades such as U71Mn or U75V, as defined by GB/T 2585. The process begins in steelmaking, where carbon, manganese and silicon are adjusted to the specified range and phosphorus and sulphur are held to a maximum of 0.025 percent each. Secondary metallurgy and vacuum or gas treatment follow, mainly to reduce hydrogen and oxygen content: hydrogen in a high carbon rail steel is the direct cause of the internal flakes that later develop into transverse fractures.

The molten steel is continuously cast into blooms under controlled cooling, and the blooms are inspected for surface defects and for segregation before rolling. A bloom with a surface crack, a scab or a heavy corner defect will carry that discontinuity into the finished rail, so scarfing and conditioning at this stage is not optional. The heat number is recorded and carried through every subsequent step, because traceability begins here.

Reheating and Rolling

Blooms are heated in a walking beam furnace to a controlled temperature, and the key process control is to avoid both an excessive temperature that produces a coarse grain structure and an excessive residence time that causes decarburisation of the surface. The discharge temperature is measured and recorded for each bloom.

Stage Function Control point
Reheating Bring bloom to rolling temperature Discharge temperature, residence time
Roughing and breakdown Reduce bloom to a bar of rail proportion Reduction schedule, temperature
Universal roughing and finishing Form head, web and base with the correct angles Roll pass geometry, web and head dimensions
Edging Set base width and head profile Asymmetry of the head
Sawing Cut to ordered length with allowance Length, squareness of the cut end

Modern lines roll the rail in a universal (four roll) pass sequence rather than in a two-high groove series, because the universal arrangement shapes the head and base simultaneously and gives better dimensional consistency along the length. The finishing temperature matters: it determines the austenite grain size at the moment the rail enters the cooling bed, and therefore the toughness of the finished product.

Cooling, Straightening and Camber

After rolling the rail is cooled on the bed under controlled conditions. Cooling too quickly through the transformation range generates internal stresses and can produce hard, brittle zones; cooling too slowly allows the austenite grain size to coarsen and reduces strength. The cooling path is therefore monitored rather than left to ambient conditions.

Straightening follows cooling. The rail passes through a series of roller straighteners that correct vertical and horizontal bow and set the specified camber, which is the slight upward curvature that offsets the deflection the rail will experience under load. Straightening introduces its own residual stress, so the sequence and the roll settings are part of the product specification, not just a workshop preference.

Heat Treatment Options for the Head

Where the duty requires more wear resistance than an as-rolled grade can provide, the head is hardened. The head is reheated by induction or by residual heat and then quenched with air and water mist at a rate that produces fine pearlite rather than martensite, followed by controlled tempering. The result is a head hardness substantially higher than the as-rolled value, with the hardened layer extending several tens of millimetres below the running surface, while the web and the base retain their original toughness.

The important point for a purchaser is that the hardness must be present at the specified measurement depth and must persist after the grinding cycles the rail will receive in track. A quotation that states only a surface hardness value does not define the product.

Inspection, Drilling and Marking

The finished rail is inspected on several fronts. Dimensional checking covers head width and asymmetry, web thickness, base width, overall height, straightness, camber and hole positions. Internal soundness is verified by ultrasonic testing over the whole length. Mechanical testing covers tensile strength and hardness, and the results are tied to the heat number.

Drilling for the joint pattern is carried out after the rail is straightened and before delivery, and the hole edges must be deburred and free from sharp corners because a sharp corner at a bolt hole is a fatigue initiation point. Finally the rail is marked with the grade, the heat number, the section, the manufacturer code and the length; without that marking the material cannot be traced once it is on site.

Frequently Asked Questions

Q: What raw material is used for 50 kg/m heavy rail?
A: Continuously cast blooms of high carbon rail steel in grades such as U71Mn or U75V, produced to the composition ranges of GB/T 2585 and conditioned to remove surface defects before rolling.

Q: Why is hydrogen control important in rail steel?
A: Hydrogen in high carbon steel causes internal flakes that act as crack initiation sites and can lead to a transverse fracture in service. Degassing and controlled casting address it.

Q: What is camber and why is it set?
A: Camber is a slight upward curvature built into the rail by the straightener to compensate for the downward deflection the rail experiences under wheel load in track.

Q: How is the rail head hardened without making it brittle?
A: The head is reheated and quenched at a rate that forms fine pearlite rather than martensite, then tempered, so hardness rises while the web and base remain tough.

Q: How is internal soundness of the finished rail checked?
A: By ultrasonic testing over the full length, supported by dimensional measurement, hardness and tensile testing, with all results linked to the heat number.

Q: Why must bolt holes be deburred?
A: A sharp corner at a drilled hole concentrates stress and becomes the initiation point for fatigue cracking, so the hole edges are deburred and the hole pattern is cut to the specified joint bar.